Features:
Nimonic alloy 90 is a precipitation hardenable nickel-chromium-cobalt alloy strengthened by the addition of Titanium and Aluminium. Alloy 90 has a high stress rupture strength and creep-resistant at temperatures to 920°C. Nimonic Alloy 90 is typically used in extreme stress applications such as turbine blades, hot working tools, exhaust reheaters, disc and high-temperature springs.
The recommended heat treatments for Nimonic 90 are as follows:
Nimonic 90 Bar
Solution Treatment - 1080 °C (1975 °F) for 8 hours + air cool or oil/ water quench
Precipitation Heat Treatment (As per BS HR2) - 700 °C (1290 °F) for 16 hours + air cool
Nimonic 90 Sheet
Solution Treatment - 1100-1150 °C for 1-10 minutes + air cool or oil /water quench
Stabilization Heat Treatment - 925 °C for 1 hour + air cool
Precipitation Heat Treatment - 750 °C for 4 hours and air cool
(BS HR202/ MSRR 7016 / Siemens TLV 85252100 do not require the Stabilization Treatment stage)
Nominal composition,%
|
Alloy designation |
C |
Ni |
Cr |
Co |
Pb |
Fe |
Al |
B |
Ti |
S |
Mn |
Cu |
Zr |
Si |
|
Alloy 90 Nimonic 90 |
0.2 |
Bal |
18~21 |
15~21 |
0.002max |
1.5 |
1~2 |
0.02 |
2~3 |
0.015 |
1 |
0.2 |
0.15 |
1 |
Typical Mechanical Properties:
|
Material Extruded Bar |
Temperature °C |
Yield Strength 0.2 % (MPa) |
Tensile Strength (MPa) |
Elongation (%) |
Hardness HV |
|
Nimonic 90 bar Solution Treated (BS HR2) |
RT |
- |
- |
- |
295max |
|
Nimonic 90 bar Precipition Treated (BS HR2) |
RT |
695MIN |
1080MIN |
20MIN |
310min |
|
Nimonic 90 Bar Precipitation Treated (BS HR2) |
500 |
672(typical) |
1038(typical) |
31 |
- |
Availability:
Nimonic Alloy 90 (Nimonic 90) is available in sheet, strip, plate, bar, round bar, flat bar, wire, forging stock, tube, welding wire and extruded section